J. Semicond. >  Just Accepted

REVIEWS

Research progress on laser stealth dicing of typical semiconductor materials

Haoyu Fan, Xing Zhang, Linlin Che, Yufeng Xue, Jiawei Wang, Yangyang Jia, Qiu Chen, Baitao Zhang, Xiufang Chen, Rongkun Wang and Xiangang Xu

+ Author Affiliations

 Corresponding author: Qiu Chen, chenqiu0629@sdu.edu.cn; Xiufang Chen, cxf@sdu.edu.cn; Rongkun Wang, wrk@sdu.edu.cn

DOI: 10.1088/1674-4926/26070048CSTR: 32376.14.1674-4926.26070048

PDF

Turn off MathJax

Abstract: Laser stealth dicing (LSD) enables low-damage wafer separation through subsurface modification and controlled crack propagation, with processing behavior strongly dependent on material properties. This review compares LSD of Si, 4H-SiC, and β-Ga2O3 in terms of energy deposition, modified-layer formation, crack propagation, and technological maturity, while recent progress in GaN and single-crystal diamond is also discussed. Si exhibits favorable near-infrared energy deposition and stable internal modification, resulting in a broad processing window and high technological maturity. In contrast, the wide bandgap, high thermal conductivity, and crystallographic anisotropy of 4H-SiC increase the modification threshold and complicate continuous modification and directional crack control. β-Ga2O3 relies more strongly on nonlinear absorption, while its low thermal conductivity and pronounced cleavage increase the risks of thermal damage and crack deflection. Recent advances in pulse regulation, focal-energy control, and multi-stage processing are summarized. Finally, key challenges in modification continuity, crack controllability, processing quality, and efficiency are discussed, providing guidance for material-specific optimization of semiconductor LSD.

Keywords: Laser stealth dicing, Semiconductor materials, Si, 4H-SiC, β-Ga2O3, GaN, Diamond, Modified layer, Crack propagation2



[1]
Yang X, Ran S H, Li Z Q, et al. Field programmable silicon microring WDM transceiver leveraging monolithically integrated phase-change materials. PhotoniX, 2025, 6(1): 16. doi: 10.1186/s43074-025-00174-7
[2]
Laryn T, Chu R J, Kim Y, et al. Multifunctional metamorphic III-V distributed Bragg reflectors grown on Si substrate for resonant cavity surface emitting devices. PhotoniX, 2025, 6(1): 21. doi: 10.1186/s43074-025-00180-9
[3]
Zheng X, Zhao G B, Dai Y R, et al. V-pit-induced electric field redistribution enabling efficient hole injection in InGaN-based red light-emitting diodes grown on silicon. PhotoniX, 2025, 6(1): 55. doi: 10.1186/s43074-025-00214-2
[4]
Choi M, Kang H, Kang D, et al. Hybrid high-index composite meta-structures with atomic layer-coated nanoparticle-embedded resin. PhotoniX, 2025, 6(1): 44. doi: 10.1186/s43074-025-00204-4
[5]
Hao Z Y, Zhang Y, Zhu Y F, et al. Compound metalens-based miniature two-photon microscope for large-FOV imaging in freely behaving animals. PhotoniX, 2025, 6(1): 57. doi: 10.1186/s43074-025-00218-y
[6]
Qiao D Y, Shi F, Tian Y, et al. Ultra-smooth polishing of single-crystal silicon carbide by pulsed-ion-beam sputtering of quantum-dot sacrificial layers. Materials, 2024, 17(1): 157. doi: 10.3390/ma17010157
[7]
Tang X, Irvine K G, Zhang D P, et al. Linear electro-optic effect in cubic silicon carbide. Appl Phys Lett, 1991, 59(16): 1938. doi: 10.1063/1.106165
[8]
Zhang X J, Zhang Z Y, Zheng L G, et al. Manufacturing and testing SiC aspherical mirrors in space telescopes. ICO20 Opt Devices Instrum, 2006, 6024: 602402.
[9]
Lin Q Y, Fan Z J, Wang W J, et al. The effect of spot overlap ratio on femtosecond laser planarization processing of SiC ceramics. Opt Laser Technol, 2020, 129: 106270. doi: 10.1016/j.optlastec.2020.106270
[10]
Cvetković S, Morsbach C, Rissing L. Ultra-precision dicing and wire sawing of silicon carbide (SiC). Microelectron Eng, 2011, 88(8): 2500. doi: 10.1016/j.mee.2011.02.026
[11]
Phillips K C, Gandhi H H, Mazur E, et al. Ultrafast laser processing of materials: A review. Adv Opt Photon, 2015, 7(4): 684. doi: 10.1364/AOP.7.000684
[12]
Watanabe W, Li Y, Itoh K. Ultrafast laser micro-processing of transparent material. Opt Laser Technol, 2016, 78: 52. doi: 10.1016/j.optlastec.2015.09.023
[13]
Wu P C, Chen C D, Hong Y, et al. Ultra-stable waveguides for on-chip integration of hBN emitters. PhotoniX, 2026, 7(1): 54. doi: 10.1186/s43074-026-00274-y
[14]
Heo J, Wi C, Chinnapaiyan N, et al. All-surface carbon circuitry enabled by ultrafast laser chemical vapor deposition. PhotoniX, 2026, 7(1): 24. doi: 10.1186/s43074-026-00243-5
[15]
Kumagai M, Uchiyama N, Ohmura E, et al. Advanced dicing technology for semiconductor wafer: Stealth dicing. IEEE Trans Semicond Manuf, 2007, 20(3): 259. doi: 10.1109/TSM.2007.901849
[16]
Takiguchi Y, Matsumoto N, Oyaizu M, et al. Improvement of laser dicing performance II: Dicing rate enhancement by multi beams and simultaneous aberration correction with phase-only spatial light modulator. Laser Based Micro Nanopackaging Assem VII, 2013, 8608: 860809.
[17]
Lawn B R. Fracture of brittle solids. 2nd ed. Cambridge: Cambridge University Press, 1993.
[18]
Chen J, Wen Q L, Yang Y, et al. Impact of crystal orientation on laser scribing and cleaving of 4H-SiC. Opt Laser Technol, 2025, 192: 114049. doi: 10.1016/j.optlastec.2025.114049
[19]
Zhang J F, Chen Y Y, Che L L, et al. Comparative study on substrate quality of laser slicing and wire saw slicing for SiC wafers. CrystEngComm, 2026, 28(1): 177. doi: 10.1039/D5CE00994D
[20]
Yang B, Wang H, Peng S, et al. Precision layered stealth dicing of SiC wafers by ultrafast lasers. Micromachines, 2022, 13(7): 1011. doi: 10.3390/mi13071011
[21]
Yan Y X, Chen S J, Cheng Y X, et al. Study on picosecond laser multi-layer modification and stealth dicing of 4H-SiC wafers based on laser power modulation. Opt Laser Technol, 2026, 198: 114882. doi: 10.1016/j.optlastec.2026.114882
[22]
Ren Y P, Tu X C, He K, et al. Study of stealth dicing of silicon carbide wafers under ultrafast laser multi-pulse mode and burst mode. Chin J Laser, 2023, 50(20): 2002405. doi: 10.3788/CJL230517
[23]
Wen Q L, Yang Y, Lu J, et al. Study on picosecond laser stealth dicing of 4H-SiC along [11 $\bar 2$0] and [1 $\bar 1$00]crystal orientations on Si-face and C-face. Opt Laser Technol, 2023, 162: 109300. doi: 10.1016/j.optlastec.2023.109300
[24]
Xie X Z, Liu T, Lv K J, et al. The internal modified layer structure of silicon carbide induced by ultrafast laser and its application in stealth dicing. Precis Eng, 2024, 88: 895. doi: 10.1016/j.precisioneng.2024.05.006
[25]
Son Y, Shin J. Laser ablation and stealth dicing of full-thickness silicon wafer. Int J Adv Manuf Technol, 2025, 137(3): 1599. doi: 10.1007/s00170-025-15275-7
[26]
Wang L F, Zhang C, Liu F, et al. Ultrafast pulsed laser stealth dicing of 4H-SiC wafer: Structure evolution and defect generation. J Manuf Process, 2022, 81: 562. doi: 10.1016/j.jmapro.2022.06.064
[27]
Sun Z P, Zou J J, Li R, et al. Laser stealth dicing of β-Ga2O3: Theoretical and experimental studies. J Mater Sci Technol, 2025, 238: 303. doi: 10.1016/j.jmst.2025.03.044
[28]
Zhang M L, Liu Z, Yang L L, et al. β-Ga2O3-based power devices: A concise review. Crystals, 2022, 12(3): 406. doi: 10.3390/cryst12030406
[29]
Okada Y, Tokumaru Y. Precise determination of lattice parameter and thermal expansion coefficient of silicon between 300 and 1500 K. J Appl Phys, 1984, 56(2): 314. doi: 10.1063/1.333965
[30]
Xu C H, Wang S C, Wang G, et al. Temperature dependence of refractive indices for 4H- and 6H-SiC. J Appl Phys, 2014, 115(11): 113501. doi: 10.1063/1.4868576
[31]
Hull R, ed. Properties of crystalline silicon. London: INSPEC, 1999.
[32]
Capan I. Electrically active defects in 3C, 4H, and 6H silicon carbide polytypes: A review. Crystals, 2025, 15(3): 255. doi: 10.3390/cryst15030255
[33]
Chiang J L, Yadlapalli B K, Chen M I, et al. A review on gallium oxide materials from solution processes. Nanomaterials, 2022, 12(20): 3601. doi: 10.3390/nano12203601
[34]
Guidry M A, Yang K Y, Lukin D M, et al. Optical parametric oscillation in silicon carbide nanophotonics. Optica, 2020, 7(9): 1139. doi: 10.1364/OPTICA.394138
[35]
Yoo J H, Rafique S, Lange A, et al. Lifetime laser damage performance of β-Ga2O3 for high power applications. APL Mater, 2018, 6(3): 036105. doi: 10.1063/1.5021603
[36]
Green M A. Self-consistent optical parameters of intrinsic silicon at 300K including temperature coefficients. Sol Energy Mater Sol Cells, 2008, 92(11): 1305. doi: 10.1016/j.solmat.2008.06.009
[37]
Bhaumik I, Bhatt R, Ganesamoorthy S, et al. Temperature-dependent index of refraction of monoclinic Ga2O3 single crystal. Appl Opt, 2011, 50(31): 6006. doi: 10.1364/AO.50.006006
[38]
Zhang Z, Wen Z D, Shi H Y, et al. Dual laser beam asynchronous dicing of 4H-SiC wafer. Micromachines, 2021, 12(11): 1331. doi: 10.3390/mi12111331
[39]
Guo Z, Verma A, Wu X F, et al. Anisotropic thermal conductivity in single crystal β-gallium oxide. Appl Phys Lett, 2015, 106(11): 111909. doi: 10.1063/1.4916078
[40]
Kumagai M, Sakamoto T, Ohmura E. Laser processing of doped silicon wafer by the Stealth Dicing. 2007 International Symposium on Semiconductor Manufacturing, 2008: 1.
[41]
Ohmura E, Kumagai M, Nakano M, et al. Analysis of processing mechanism in stealth dicing of ultra thin silicon wafer. J Adv Mech Des Syst Manuf, 2008, 2(4): 540.
[42]
Li J, Liu B, Zhang Y. Dual-stage temporal laser stealth dicing of silicon carbide wafers with continuous crack propagation. Mater Sci Semicond Process, 2026, 201: 110067. doi: 10.1016/j.mssp.2025.110067
[43]
Orlandi F, Mezzadri F, Calestani G, et al. Thermal expansion coefficients of β-Ga2O3 single crystals. Appl Phys Express, 2015, 8(11): 111101. doi: 10.7567/APEX.8.111101
[44]
Gattass R R, Mazur E. Femtosecond laser micromachining in transparent materials. Nat Photonics, 2008, 2(4): 219. doi: 10.1038/nphoton.2008.47
[45]
Stuart B C, Feit M D, Rubenchik A M, et al. Laser-induced damage in dielectrics with nanosecond-to-subpicosecond pulses. 1995, CFD2.
[46]
Li H O, Wei C R, Wang X F, et al. Research progress on wafer laser cutting technology. Semicond Technol, 2017, 42(8): 561
[47]
Suzuki N, Ohba T, Kondo Y, et al. High throughput and improved edge straightness for memory applications using stealth dicing. 2018 IEEE 68th Electronic Components and Technology Conference (ECTC), 2018: 2180.
[48]
Nara Y, Kiyota H. Stealth Dicing technology with SWIR laser realizing high throughput Si wafer dicing. Laser-based Micro- and Nanoprocessing XII, 2018: 3.
[49]
Monodane T. Thermo-elastic-plastic analysis on internal processing phenomena of single-crystal silicon by nanosecond laser. J Laser Micro, 2006, 1(3): 231. doi: 10.2961/jlmn.2006.03.0016
[50]
Nara Y, Kiyota H. Direct observation of internal void formations in stealth dicing. Proc SPIE, 2018, 10520: 105200D.
[51]
Ohmura E, Kumagai M, Nakano M, et al. Analysis of processing mechanism in stealth dicing of ultra thin silicon wafer. Proc Int Conf Lead Edge Manuf 21st Century LEM21, 2007: 2007.4, 9D435.
[52]
Weakliem H A, Redfield D. Temperature dependence of the optical properties of silicon. J Appl Phys, 1979, 50(3): 1491. doi: 10.1063/1.326135
[53]
Fukuyo F, Ohmura E, Fukumitsu K, et al. Measurement of temperature dependences of absorption coefficient of single crystal silicon. J Jpn Laser Process Soc, 2007, 14(1): 22
[54]
Lin J W, Cheng M H. Investigation of chipping and wear of silicon wafer dicing. J Manuf Process, 2014, 16(3): 373. doi: 10.1016/j.jmapro.2014.04.002
[55]
Yuan Z W, Feng S, Wu T Z. Preparation and characterization of ultra-thin dicing blades with different bonding properties. Int J Adv Manuf Technol, 2022, 119(9): 6819. doi: 10.21203/rs.3.rs-997935/v1
[56]
Zhao Z H, Zhou X Y, Du C P, et al. Stress analysis of ultrafast-laser stealth dicing and high-efficiency dicing process for complex wafer structures. Chin J Laser, 2026, 53(8): 0802506. doi: 10.3788/CJL250651
[57]
Song Q, Zhang Z, Xu Z Y, et al. Investigation on the processing quality of nanosecond laser stealth dicing for 4H-SiC wafer. ECS J Solid State Sci Technol, 2023, 12(3): 033012. doi: 10.1149/2162-8777/acc135
[58]
Song Y G, Guo X, Wang Y L, et al. Research on stealth dicing silicon carbide wafer by picosecond laser pulses. Opt Instrum, 2022, 44(3): 88.
[59]
Meyer R, Froehly L, Giust R, et al. Extremely high-aspect-ratio ultrafast Bessel beam generation and stealth dicing of multi-millimeter thick glass. Appl Phys Lett, 2019, 114(20): 201105. doi: 10.1063/1.5096868
[60]
Galazka Z, Uecker R, Irmscher K, et al. Czochralski growth and characterization of β-Ga2O3 single crystals. Cryst Res Technol, 2010, 45(12): 1229. doi: 10.1002/crat.201000341
[61]
Yang J J, Chen H, Liu J X, et al. Ablation characteristics and material removal mechanism of a β-Ga2O3 processed by picosecond laser. Mater Sci Semicond Process, 2024, 173: 108136. doi: 10.1016/j.mssp.2024.108136
[62]
Lenzner M, Krüger J, Kautek W, et al. Incubation of laser ablation in fused silica with 5-fs pulses. Appl Phys A, 1999, 69(4): 465.
[63]
Zhang K, Xu Z W, Dong B, et al. Process exploration of β-Ga2O3 blind hole processing by water-assisted femtosecond laser technology. J Alloys Compd, 2023, 939: 168769. doi: 10.1016/j.jallcom.2023.168769
[64]
Zhang K, Xu Z W, Wang H, et al. Patterning the surface structure of transparent hard-brittle material β-Ga2O3 by ultrashort pulse laser. Ceram Int, 2022, 48(19): 27650. doi: 10.1016/j.ceramint.2022.06.061
[65]
Ahn M, Sarracino A, Ansari A, et al. Unique material modifications of Ga2O3 enabled by ultrafast laser irradiation. Oxide-based Materials and Devices XI, 2020: 20.
[66]
Zhang H B, Eaton S M, Herman P R. Low-loss Type II waveguide writing in fused silica with single picosecond laser pulses. Opt Express, 2006, 14(11): 4826. doi: 10.1364/oe.14.004826
[67]
McMillen B, Zhang B T, Chen K, et al. Ultrafast laser fabrication of low-loss waveguides in chalcogenide glass with 0.65 dB/cm loss. 2012 Conference on Lasers and Electro-Optics (CLEO), 2012: 1.
[68]
Soltani B, Azarhoushang B, Zahedi A. Laser ablation mechanism of silicon nitride with nanosecond and picosecond lasers. Opt Laser Technol, 2019, 119: 105644. doi: 10.1016/j.optlastec.2019.105644
[69]
Wright E M, Koch S W, Kolesik M, et al. Memory effects in the long-wave infrared avalanche ionization of gases: A review of recent progress. Rep Prog Phys, 2019, 82(6): 064401. doi: 10.1088/1361-6633/ab1a07
[70]
Kim T, Bhargava P, Poulton C V, et al. A single-chip optical phased array in a wafer-scale silicon photonics/CMOS 3D-integration platform. IEEE J Solid State Circuits, 2019, 54(11): 3061. doi: 10.1109/JSSC.2019.2934601
[71]
Seok T J, Kwon K, Henriksson J, et al. Wafer-scale silicon photonic switches beyond die size limit. Optica, 2019, 6(4): 490. doi: 10.1364/OPTICA.6.000490
[72]
Lin J J, You T G, Jin T T, et al. Wafer-scale heterogeneous integration InP on trenched Si with a bubble-free interface. APL Mater, 2020, 8(5): 051110. doi: 10.1063/5.0004427
[73]
Hollenbach M, Klingner N, Jagtap N S, et al. Wafer-scale nanofabrication of telecom single-photon emitters in silicon. Nat Commun, 2022, 13: 7683. doi: 10.1038/s41467-022-35051-5
[74]
Jo G, Edinger P, Bleiker S J, et al. Wafer-level hermetically sealed silicon photonic MEMS. Photon Res, 2022, 10(2): A14. doi: 10.1364/PRJ.441215
[75]
Zhang J, Dong P, Dang K, et al. Ultra-wide bandgap semiconductor Ga2O3 power diodes. Nat Commun, 2022, 13: 3900. doi: 10.1038/s41467-022-31664-y
[76]
Labed M, Sengouga N, Prasad C V, et al. On the nature of majority and minority traps in β-Ga2O3: A review. Mater Today Phys, 2023, 36: 101155. doi: 10.1016/j.mtphys.2023.101155
[77]
Sun Z P, Zhang D L, Qi Z J, et al. Insight into interfacial heat transfer of β-Ga(2)O(3)/diamond heterostructures via the machine learning potential. ACS Appl Mater Interfaces, 2024, 16(24): 31666. doi: 10.1021/acsami.3c19588
[78]
Higashiwaki M, Sasaki K, Kuramata A, et al. Development of gallium oxide power devices. Phys Status Solidi A, 2014, 211: 21-26. doi: 10.1002/pssa.201330197
[79]
Shan F K, Liu G X, Lee W J, et al. Structural, electrical, and optical properties of transparent gallium oxide thin films grown by plasma-enhanced atomic layer deposition. J Appl Phys, 2005, 98(2): 023504 doi: 10.1063/1.1980535
[80]
Yoshioka S, Hayashi H, Kuwabara A, et al. Structures and energetics of Ga2O3. J Phys Condens Matter, 2007, 19(34): 346211. doi: 10.1088/0953-8984/19/34/346211
[81]
Roy R, Hill V G, Osborn E F. Polymorphism of Ga2O3 and the system Ga2O3: H2O. J Am Chem Soc, 1952, 74(3): 719.
[82]
Reese S B, Remo T, Green J, et al. How much will gallium oxide power electronics cost? Joule, 2019, 3(4): 903.
[83]
Schaffer C B, Brodeur A, Mazur E. Laser-induced breakdown and damage in bulk transparent materials induced by tightly focused femtosecond laser pulses. Meas Sci Technol, 2001, 12(11): 1784. doi: 10.1088/0957-0233/12/11/305
[84]
Jiang L, Wang A D, Li B, et al. Electrons dynamics control by shaping femtosecond laser pulses in micro/nanofabrication: Modeling, method, measurement and application. Light Sci Appl, 2018, 7(2): 17134. doi: 10.1038/lsa.2017.134
[85]
Chen J L, Lu X Z, Li Z, et al. Anisotropy of material removal during laser-induced plasma assisted ablation of sapphire. Ceram Int, 2022, 48(10): 13880. doi: 10.1016/j.ceramint.2022.01.272
[86]
Lei M L, Meng L H, Lin Y C, et al. Stealth dicing strategy for fabricating the cleavage mirror facets of semiconductor laser. Mater Des, 2025, 251: 113695. doi: 10.1016/j.matdes.2025.113695
[87]
Parks S M, Grote R R, Hopper D A, et al. Fabrication of (111)-faced single-crystal diamond plates by laser nucleated cleaving. Diam Relat Mater, 2018, 84: 20. doi: 10.1016/j.diamond.2018.02.013
[88]
Mu C Y, Lv X Y, Wang Q L, et al. Mosaic growth and characteristics of 2-inch single-crystal diamond. Funct Diam, 2026, 6(1): 2620820. doi: 10.1080/26941112.2026.2620820
[89]
Onishi K, Kitagawa H, Teranishi S, et al. Temporary direct bonding by low temperature deposited SiO2 for chiplet applications. ACS Appl Electron Mater, 2024, 6(4): 2449. doi: 10.1021/acsaelm.4c00114
[90]
Inoue F, Podpod A, Peng L, et al. Morphological characterization and mechanical behavior by dicing and thinning on direct bonded Si wafer. J Manuf Process, 2020, 58: 811. doi: 10.1016/j.jmapro.2020.08.050
[91]
Windemuth R. Plasma dicing for thin wafers. 2015 European Microelectronics Packaging Conference (EMPC), 2016: 1.
[92]
Pushpakaran B N, Subburaj A S, Bayne S B, et al. Impact of silicon carbide semiconductor technology in Photovoltaic Energy System. Renew Sustain Energy Rev, 2016, 55: 971. doi: 10.1016/j.rser.2015.10.161
[93]
Cunningham D W, Carlson E P, Manser J S, et al. Impacts of wide band gap power electronics on photovoltaic system design. IEEE J Photovolt, 2020, 10(1): 213. doi: 10.1109/JPHOTOV.2019.2950592
[94]
Robles E, Matallana A, Aretxabaleta I, et al. The role of power device technology in the electric vehicle powertrain. Int J Energy Res, 2022, 46(15): 22222. doi: 10.1002/er.8581
[95]
Liu G Y, Wu Y B, Li K J, et al. Development of high power SiC devices for rail traction power systems. J Cryst Growth, 2019, 507: 442. doi: 10.1016/j.jcrysgro.2018.10.037
Fig. 1.  Comparison of results between traditional dicing and laser stealth dicing [16]

Fig. 2.  (Color online) Representative laser stealth dicing processes and applications of the three principal material systems discussed in this review: Si, 4H-SiC, and β-Ga2O3[15, 23, 25−27].

Fig. 3.  (Color online) Comparison of selected properties of three semiconductor materials.

Fig. 4.  (Color online) Schematic of the Si crystal structure, with representative crystallographic planes and directions relevant to crack propagation. The inset legend identifies the Si atoms.

Fig. 5.  Schematic diagram of the principle of stealth dicing technology[15]

Fig. 6.  (Color online) Side view of a 775 μm thick Si wafer cut using three wavelengths. (a) 1064 nm; (b) 1080 nm; (c) 1099 nm[47],and comparison of process result at high throughput SDE with aberration correction and SWIR laser to conventional SDE (d)-(g)[48].

Fig. 7.  (Color online) Temperature dependence of absorption coefficient of silicon single crystal for 1064 nm[52, 53]

Fig. 8.  (Color online) Schematic diagram of the laser processing apparatus[56]

Fig. 9.  (Color online) Schematic of the 4H-SiC crystal structure, showing representative crystallographic planes and directions associated with orientation-dependent crack propagation during laser stealth dicing. The inset legend identifies Si and C atoms.

Fig. 10.  (a) Illustration of laser processing step in the LSD method. (b) Illustration of LSD layer and crack after laser processing step[40]

Fig. 11.  (Color online) (a) and (b) Surface morphologies of Si-face and C-face of 4H-SiC samples. (c) and (d) Schematic diagram of the crystal orientations of Si-face and C-face of 4H-SiC samples, respectively[23]. Cross sections of the PLSD kerfs along different crystal orientations or planes. (e) The crosssection of crystal plane (10-10) and (f) the cross section of crystal plane (11-20)[20].

Fig. 12.  (Color online) (a) PLSD[20]; (b) schematic diagram of internal modification layer processing in 4H-SiC [57]; (c) SEM images of the cross-sectional edge without and with laser power modulation; (d) cross-sectional roughness as a function of the power-modulation parameter ω[21].

Fig. 13.  (Color online) (a)−(c)The evolution process of the modified layer at different moving velocities.(d)−(f)The average surface roughness of the LSD cross-section and the critical fracture load of the 4H–SiC wafer under three modified layer structures[24]

Fig. 14.  (Color online) The DLSD method and experiments (a) schematic diagram of the DLSD method, (b) modified laser generates modified layer, (c) induced laser promotes crack propagation, (d) optical system and processing platform, (e) wafer separation method[42]. Configuration of a dual laser beam asynchronous dicing system: (f) schematic diagram of experimental set-up; (g) experimental platform with dual laser path[38]

Fig. 15.  (Color online) Effect of the number of sub-pulses on the stealth-dicing quality of 4H-SiC under burst mode: (a–d) cross-sectional morphologies obtained with different numbers of sub-pulses; (e) variations in upper- and lower-surface edge-chipping size and cross-sectional roughness with the number of sub-pulses [22].

Fig. 16.  (Color online) Schematic diagram of the β-Ga2O3 crystal structure

Fig. 17.  (Color online) (a) schematic diagram of Gaussian laser machining. (b) 3D morphology of AFM-scanned grooves and measurement of width and depth. Section profile under different (c) single pulse energies, (d) laser scanning speeds.(e) Schematic diagram of the picosecond laser-processing system[61]

Fig. 18.  (Color online) (a) Schematic diagram and (b) three-dimensional MD model of β-Ga2O3[27]

Fig. 19.  (Color online) Experimental fracture-surface characteristics of β-Ga2O3 after laser stealth dicing: fracture-surface morphologies of the (a) (100), (b) (010), and (c) (001) planes at a laser repetition rate of 100 kHz; (d) comparison of the arithmetic mean height (Sa) of the fracture surfaces at different repetition rates [27].

Table 1.   Quantitative comparison of representative wafer dicing technologies.

Dicing methodProcessing efficiencyMaterial loss /
kerf width
Cross-sectional roughnessEdge chippingSubsurface / thermal damageMain advantages and limitations
Diamond-blade dicingFeed rate 0.3 mm s−1 [10]another reported SiC process: 1 mms−1[17]Kerf width
201–214 μm[17]; conventional
thick-blade SiC dicing approximately 200 μm[10, 17]
Sidewall roughness 185 nm[10]Maximum edge chipping 60 μm[10]Mechanical contact can induce chipping, cracking and residual/subsurface damage[10]Mature and accurate, but suffers from tool wear, relatively large kerf loss and mechanical damage[10]
Diamond-wire sawingsawingFor 8-inch 4H-SiC: ≈45 min wafer−1[18]Material loss
≈240 μm wafer−1[18]
As-sawn 8-inch 4H-SiC: Ra = 0.286 μm[18]Not reported quantitatively under the same conditions; brittle-fracture-induced defects may occur[10, 18]Mechanical damage and microcracks are present in the as-sawn surface[10, 18]Suitable for ingot slicing and mature industrial processing, but material loss and mechanical damage remain significant[18]
Surface-ablation laser cuttingRepresentative SiC full-dicing condition:
4 mm s−1, 12 scanning passes[19]
Kerf width
≈15 μm[19]
Cross-sectional roughness
Ra =296nm[19]
No reliable quantitative value reported in the selected study; fracture-surface microcracks decrease as roughness decreases[19]Excessive pulse energy causes over-ablation and SiO2 redeposition[19]Non-contact and narrow kerf, but direct material removal can cause redeposition, thermal effects and requires repeated scans[19]
Laser stealth dicing (LSD)PLSD scanning speed 10 mm*s−1[20]; multilayer modification provides >4× the processing efficiency of single-layer modification[21]No continuous ablation kerf is required; material removal is strongly suppressed[15, 20]PLSD: about 1 μm[20]; power-modulated multilayer LSD:
Sa = 362 nm[21]
Burst-mode 4H-SiC: 1.2 μm top / 1.0 μm bottom[22]Localized modified layers and microcracks are intentionally generated; uncontrolled internal cracking remains possible[20−22]Dry, non-contact and low-loss separation with reduced surface damage; limited by optical accessibility, focal-energy control and crack-propagation stability[15, 20−22]
The quantitative values are representative results reported in the literature and were not obtained under identical experimental conditions. They depend on wafer material, thickness, crystallographic orientation, tool geometry, laser parameters, and evaluation methods. Therefore, the values are intended to provide a quantitative indication of the characteristic performance of different dicing strategies rather than a strict one-to-one ranking.
DownLoad: CSV

Table 2.   Comparison of key physical properties relevant to stealth dicing for the three principal material systems: Si, 4H-SiC, and β-Ga2O3.

PropertySi4H-SiCβ-Ga2O3
Bandgap (eV, ~300 K)1.12[28]3.26−3.28[29]4.8−4.9[30]
Optical response at 1064 nm~10 cm−1 [31]0.031–0.063 dB·cm−1* [32]T≈ 70.4%** [33]
Refractive index, (~1064 nm, RT)~3.5[31]~2.6 [34]~1.9[35]
Thermal conductivity, k (W·m−1·K−1, RT)~150 [36]~350–490* [29]10.9−27.0[37]*
Thermal expansion coefficient (10−6 K−1)2.63[36]≈4.3 [38]1.54–3.37[39]*
Melting/decomposition temperature (°C)1414 [28]
≈2500–2800, decomposition/sublimation [29]≈1790–1800[30]
Crystal structureDiamond cubic [28]Hexagonal (4H) [29]Monoclinic [30]
*Values are representative literature data. Thermal properties are given at approximately room temperature unless otherwise specified, and optical properties are reported at or near 1064 nm. Crystallographic directions or polarization states are specified for anisotropic properties where applicable. The 1064-nm optical loss of 4H-SiC corresponds to HPSI 4H-SiC, whereas the β-Ga2O3 transmittance (70.4%) corresponds to a 680-μm-thick Sn-doped (2ˉ01) bulk single crystal. For SiC, the listed high-temperature value represents the decomposition/sublimation range rather than a conventional melting point.
DownLoad: CSV

Table 3.   Representative critical processing parameters and strategies for laser stealth dicing of semiconductor materials discussed in this review.

Material Processing strategy Sample / wafer Laser parameters Energy / power Scanning / focusing condition Representative processing result Source
Si Wavelength-dependent conventional LSD 775−μm−thick Si wafer 1064, 1080, and 1099 nm / Internal focusing The 1099-nm laser generated longer cracks, whereas 1064 nm produced the shortest crack extension beneath the modified layer [47]
Si SWIR-LSD with spherical-aberration correction Si wafer 1064 and 1342 nm / 1064 nm: 7 scans; 1342 nm: 3 scans; 1342 nm with aberration correction: 2 scans Longer-wavelength irradiation and aberration correction reduced the number of scans required for wafer separation [48]
4H-SiC Hundred-picosecond LSD 4H-SiC wafer 1030 nm; ~100 ps; 100 kHz 20 μJ pulse−1 200, 400, and
800 mm∙s−1; optimum condition reported at 400 mm∙s−1
At 400 mm∙s−1, the modified-point spacing was ~4 μm, producing a flat cross-section without obvious edge chipping [58]
4H-SiC Precision layered stealth dicing (PLSD) 508-μm-thick semi-insulating 4H-SiC wafer 5 ps; 200 kHz 45 μJ pulse−1; 9 W 10 mm∙s−1; bottom-to-top multilayer scanning; 100× objective, NA = 0.7 Depth-dependent layered modification enabled a continuous weakened region through the thick wafer [20]
4H-SiC Power-modulated multilayer LSD 500-μm-thick semi-insulating 4H-SiC wafer 1064 nm; 10 ps; 10 kHz under the representative modification condition 100 mW for single-layer modification; 300 mW for multilayer modification; optimized modulation parameter ω = 2.8 50 mm s−1; multilayer scanning with spatial power modulation Power modulation reduced cross-sectional roughness from 583 to 362 nm while maintaining the high efficiency of multilayer modification [21]
4H-SiC Dual-beam asynchronous dicing (DBAD) 200-μm-thick 4H-SiC wafer Pulsed laser:
532 nm, 750 fs, 20–200 kHz; CW laser: 1040 nm
Pulsed laser ≤5 W; CW laser ≤10 W Pulsed-laser scanning speed: 3000 μm s−1; CW laser subsequently scanned along the modified path Internal modification and thermally driven crack propagation were decoupled, allowing wafer separation without the conventional mechanical breaking step [38]
4H-SiC Dual-stage laser stealth dicing (DLSD) 4H-SiC wafer Two-stage sequential laser irradiation Modifying laser: 0.14 W; inducing laser: 0.18 W 800 mm s−1; two laser passes along the same trajectory Continuous crack propagation was promoted; maximum chipping width and sidewall roughness were reduced to 6.0 and 1.15 μm, respectively [42]
4H-SiC Burst-mode LSD 4H-SiC wafer Burst-mode ultrafast pulses Constant single-pulse energy; number of sub-pulses varied Multi-pulse / burst temporal-energy modulation; optimized condition with five sub-pulses Upper- and lower-surface chipping were reduced to ~1.2 and ~1.0 μm, respectively, with a minimum cross-sectional roughness of ~2.3 μm [22]
β-Ga2O₃ Picosecond laser surface processing as a precursor to LSD Polished β-Ga2O₃ single crystal Picosecond laser Single-pulse energy varied Line scanning along the (100) direction; scanning speed and number of passes varied Established the relationship among pulse energy, pulse overlap, thermal accumulation, and processing threshold, providing a parameter basis for subsequent internal modification [61]
β-Ga2O₃ Laser stealth dicing β-Ga2O₃ wafers with (100), (010), and (001) fracture planes 1028 nm; picosecond laser; 50–200 kHz Single-pulse energy regulated mainly by repetition rate Internal focusing; crystallographic orientation and repetition rate jointly varied Fracture-surface quality showed strong orientation and repetition-rate dependence, with the (100) plane exhibiting the best surface quality under representative conditions [27]
Note: The processing parameters listed above are representative values reported in individual studies and were not obtained under identical experimental conditions. Differences in wafer thickness, crystallographic orientation, optical configuration, focal depth, and evaluation method should therefore be considered when comparing the reported processing windows. “—” indicates that the corresponding parameter was not explicitly required for the comparison or was not reported in the cited study.
DownLoad: CSV
[1]
Yang X, Ran S H, Li Z Q, et al. Field programmable silicon microring WDM transceiver leveraging monolithically integrated phase-change materials. PhotoniX, 2025, 6(1): 16. doi: 10.1186/s43074-025-00174-7
[2]
Laryn T, Chu R J, Kim Y, et al. Multifunctional metamorphic III-V distributed Bragg reflectors grown on Si substrate for resonant cavity surface emitting devices. PhotoniX, 2025, 6(1): 21. doi: 10.1186/s43074-025-00180-9
[3]
Zheng X, Zhao G B, Dai Y R, et al. V-pit-induced electric field redistribution enabling efficient hole injection in InGaN-based red light-emitting diodes grown on silicon. PhotoniX, 2025, 6(1): 55. doi: 10.1186/s43074-025-00214-2
[4]
Choi M, Kang H, Kang D, et al. Hybrid high-index composite meta-structures with atomic layer-coated nanoparticle-embedded resin. PhotoniX, 2025, 6(1): 44. doi: 10.1186/s43074-025-00204-4
[5]
Hao Z Y, Zhang Y, Zhu Y F, et al. Compound metalens-based miniature two-photon microscope for large-FOV imaging in freely behaving animals. PhotoniX, 2025, 6(1): 57. doi: 10.1186/s43074-025-00218-y
[6]
Qiao D Y, Shi F, Tian Y, et al. Ultra-smooth polishing of single-crystal silicon carbide by pulsed-ion-beam sputtering of quantum-dot sacrificial layers. Materials, 2024, 17(1): 157. doi: 10.3390/ma17010157
[7]
Tang X, Irvine K G, Zhang D P, et al. Linear electro-optic effect in cubic silicon carbide. Appl Phys Lett, 1991, 59(16): 1938. doi: 10.1063/1.106165
[8]
Zhang X J, Zhang Z Y, Zheng L G, et al. Manufacturing and testing SiC aspherical mirrors in space telescopes. ICO20 Opt Devices Instrum, 2006, 6024: 602402.
[9]
Lin Q Y, Fan Z J, Wang W J, et al. The effect of spot overlap ratio on femtosecond laser planarization processing of SiC ceramics. Opt Laser Technol, 2020, 129: 106270. doi: 10.1016/j.optlastec.2020.106270
[10]
Cvetković S, Morsbach C, Rissing L. Ultra-precision dicing and wire sawing of silicon carbide (SiC). Microelectron Eng, 2011, 88(8): 2500. doi: 10.1016/j.mee.2011.02.026
[11]
Phillips K C, Gandhi H H, Mazur E, et al. Ultrafast laser processing of materials: A review. Adv Opt Photon, 2015, 7(4): 684. doi: 10.1364/AOP.7.000684
[12]
Watanabe W, Li Y, Itoh K. Ultrafast laser micro-processing of transparent material. Opt Laser Technol, 2016, 78: 52. doi: 10.1016/j.optlastec.2015.09.023
[13]
Wu P C, Chen C D, Hong Y, et al. Ultra-stable waveguides for on-chip integration of hBN emitters. PhotoniX, 2026, 7(1): 54. doi: 10.1186/s43074-026-00274-y
[14]
Heo J, Wi C, Chinnapaiyan N, et al. All-surface carbon circuitry enabled by ultrafast laser chemical vapor deposition. PhotoniX, 2026, 7(1): 24. doi: 10.1186/s43074-026-00243-5
[15]
Kumagai M, Uchiyama N, Ohmura E, et al. Advanced dicing technology for semiconductor wafer: Stealth dicing. IEEE Trans Semicond Manuf, 2007, 20(3): 259. doi: 10.1109/TSM.2007.901849
[16]
Takiguchi Y, Matsumoto N, Oyaizu M, et al. Improvement of laser dicing performance II: Dicing rate enhancement by multi beams and simultaneous aberration correction with phase-only spatial light modulator. Laser Based Micro Nanopackaging Assem VII, 2013, 8608: 860809.
[17]
Lawn B R. Fracture of brittle solids. 2nd ed. Cambridge: Cambridge University Press, 1993.
[18]
Chen J, Wen Q L, Yang Y, et al. Impact of crystal orientation on laser scribing and cleaving of 4H-SiC. Opt Laser Technol, 2025, 192: 114049. doi: 10.1016/j.optlastec.2025.114049
[19]
Zhang J F, Chen Y Y, Che L L, et al. Comparative study on substrate quality of laser slicing and wire saw slicing for SiC wafers. CrystEngComm, 2026, 28(1): 177. doi: 10.1039/D5CE00994D
[20]
Yang B, Wang H, Peng S, et al. Precision layered stealth dicing of SiC wafers by ultrafast lasers. Micromachines, 2022, 13(7): 1011. doi: 10.3390/mi13071011
[21]
Yan Y X, Chen S J, Cheng Y X, et al. Study on picosecond laser multi-layer modification and stealth dicing of 4H-SiC wafers based on laser power modulation. Opt Laser Technol, 2026, 198: 114882. doi: 10.1016/j.optlastec.2026.114882
[22]
Ren Y P, Tu X C, He K, et al. Study of stealth dicing of silicon carbide wafers under ultrafast laser multi-pulse mode and burst mode. Chin J Laser, 2023, 50(20): 2002405. doi: 10.3788/CJL230517
[23]
Wen Q L, Yang Y, Lu J, et al. Study on picosecond laser stealth dicing of 4H-SiC along [11 $\bar 2$0] and [1 $\bar 1$00]crystal orientations on Si-face and C-face. Opt Laser Technol, 2023, 162: 109300. doi: 10.1016/j.optlastec.2023.109300
[24]
Xie X Z, Liu T, Lv K J, et al. The internal modified layer structure of silicon carbide induced by ultrafast laser and its application in stealth dicing. Precis Eng, 2024, 88: 895. doi: 10.1016/j.precisioneng.2024.05.006
[25]
Son Y, Shin J. Laser ablation and stealth dicing of full-thickness silicon wafer. Int J Adv Manuf Technol, 2025, 137(3): 1599. doi: 10.1007/s00170-025-15275-7
[26]
Wang L F, Zhang C, Liu F, et al. Ultrafast pulsed laser stealth dicing of 4H-SiC wafer: Structure evolution and defect generation. J Manuf Process, 2022, 81: 562. doi: 10.1016/j.jmapro.2022.06.064
[27]
Sun Z P, Zou J J, Li R, et al. Laser stealth dicing of β-Ga2O3: Theoretical and experimental studies. J Mater Sci Technol, 2025, 238: 303. doi: 10.1016/j.jmst.2025.03.044
[28]
Zhang M L, Liu Z, Yang L L, et al. β-Ga2O3-based power devices: A concise review. Crystals, 2022, 12(3): 406. doi: 10.3390/cryst12030406
[29]
Okada Y, Tokumaru Y. Precise determination of lattice parameter and thermal expansion coefficient of silicon between 300 and 1500 K. J Appl Phys, 1984, 56(2): 314. doi: 10.1063/1.333965
[30]
Xu C H, Wang S C, Wang G, et al. Temperature dependence of refractive indices for 4H- and 6H-SiC. J Appl Phys, 2014, 115(11): 113501. doi: 10.1063/1.4868576
[31]
Hull R, ed. Properties of crystalline silicon. London: INSPEC, 1999.
[32]
Capan I. Electrically active defects in 3C, 4H, and 6H silicon carbide polytypes: A review. Crystals, 2025, 15(3): 255. doi: 10.3390/cryst15030255
[33]
Chiang J L, Yadlapalli B K, Chen M I, et al. A review on gallium oxide materials from solution processes. Nanomaterials, 2022, 12(20): 3601. doi: 10.3390/nano12203601
[34]
Guidry M A, Yang K Y, Lukin D M, et al. Optical parametric oscillation in silicon carbide nanophotonics. Optica, 2020, 7(9): 1139. doi: 10.1364/OPTICA.394138
[35]
Yoo J H, Rafique S, Lange A, et al. Lifetime laser damage performance of β-Ga2O3 for high power applications. APL Mater, 2018, 6(3): 036105. doi: 10.1063/1.5021603
[36]
Green M A. Self-consistent optical parameters of intrinsic silicon at 300K including temperature coefficients. Sol Energy Mater Sol Cells, 2008, 92(11): 1305. doi: 10.1016/j.solmat.2008.06.009
[37]
Bhaumik I, Bhatt R, Ganesamoorthy S, et al. Temperature-dependent index of refraction of monoclinic Ga2O3 single crystal. Appl Opt, 2011, 50(31): 6006. doi: 10.1364/AO.50.006006
[38]
Zhang Z, Wen Z D, Shi H Y, et al. Dual laser beam asynchronous dicing of 4H-SiC wafer. Micromachines, 2021, 12(11): 1331. doi: 10.3390/mi12111331
[39]
Guo Z, Verma A, Wu X F, et al. Anisotropic thermal conductivity in single crystal β-gallium oxide. Appl Phys Lett, 2015, 106(11): 111909. doi: 10.1063/1.4916078
[40]
Kumagai M, Sakamoto T, Ohmura E. Laser processing of doped silicon wafer by the Stealth Dicing. 2007 International Symposium on Semiconductor Manufacturing, 2008: 1.
[41]
Ohmura E, Kumagai M, Nakano M, et al. Analysis of processing mechanism in stealth dicing of ultra thin silicon wafer. J Adv Mech Des Syst Manuf, 2008, 2(4): 540.
[42]
Li J, Liu B, Zhang Y. Dual-stage temporal laser stealth dicing of silicon carbide wafers with continuous crack propagation. Mater Sci Semicond Process, 2026, 201: 110067. doi: 10.1016/j.mssp.2025.110067
[43]
Orlandi F, Mezzadri F, Calestani G, et al. Thermal expansion coefficients of β-Ga2O3 single crystals. Appl Phys Express, 2015, 8(11): 111101. doi: 10.7567/APEX.8.111101
[44]
Gattass R R, Mazur E. Femtosecond laser micromachining in transparent materials. Nat Photonics, 2008, 2(4): 219. doi: 10.1038/nphoton.2008.47
[45]
Stuart B C, Feit M D, Rubenchik A M, et al. Laser-induced damage in dielectrics with nanosecond-to-subpicosecond pulses. 1995, CFD2.
[46]
Li H O, Wei C R, Wang X F, et al. Research progress on wafer laser cutting technology. Semicond Technol, 2017, 42(8): 561
[47]
Suzuki N, Ohba T, Kondo Y, et al. High throughput and improved edge straightness for memory applications using stealth dicing. 2018 IEEE 68th Electronic Components and Technology Conference (ECTC), 2018: 2180.
[48]
Nara Y, Kiyota H. Stealth Dicing technology with SWIR laser realizing high throughput Si wafer dicing. Laser-based Micro- and Nanoprocessing XII, 2018: 3.
[49]
Monodane T. Thermo-elastic-plastic analysis on internal processing phenomena of single-crystal silicon by nanosecond laser. J Laser Micro, 2006, 1(3): 231. doi: 10.2961/jlmn.2006.03.0016
[50]
Nara Y, Kiyota H. Direct observation of internal void formations in stealth dicing. Proc SPIE, 2018, 10520: 105200D.
[51]
Ohmura E, Kumagai M, Nakano M, et al. Analysis of processing mechanism in stealth dicing of ultra thin silicon wafer. Proc Int Conf Lead Edge Manuf 21st Century LEM21, 2007: 2007.4, 9D435.
[52]
Weakliem H A, Redfield D. Temperature dependence of the optical properties of silicon. J Appl Phys, 1979, 50(3): 1491. doi: 10.1063/1.326135
[53]
Fukuyo F, Ohmura E, Fukumitsu K, et al. Measurement of temperature dependences of absorption coefficient of single crystal silicon. J Jpn Laser Process Soc, 2007, 14(1): 22
[54]
Lin J W, Cheng M H. Investigation of chipping and wear of silicon wafer dicing. J Manuf Process, 2014, 16(3): 373. doi: 10.1016/j.jmapro.2014.04.002
[55]
Yuan Z W, Feng S, Wu T Z. Preparation and characterization of ultra-thin dicing blades with different bonding properties. Int J Adv Manuf Technol, 2022, 119(9): 6819. doi: 10.21203/rs.3.rs-997935/v1
[56]
Zhao Z H, Zhou X Y, Du C P, et al. Stress analysis of ultrafast-laser stealth dicing and high-efficiency dicing process for complex wafer structures. Chin J Laser, 2026, 53(8): 0802506. doi: 10.3788/CJL250651
[57]
Song Q, Zhang Z, Xu Z Y, et al. Investigation on the processing quality of nanosecond laser stealth dicing for 4H-SiC wafer. ECS J Solid State Sci Technol, 2023, 12(3): 033012. doi: 10.1149/2162-8777/acc135
[58]
Song Y G, Guo X, Wang Y L, et al. Research on stealth dicing silicon carbide wafer by picosecond laser pulses. Opt Instrum, 2022, 44(3): 88.
[59]
Meyer R, Froehly L, Giust R, et al. Extremely high-aspect-ratio ultrafast Bessel beam generation and stealth dicing of multi-millimeter thick glass. Appl Phys Lett, 2019, 114(20): 201105. doi: 10.1063/1.5096868
[60]
Galazka Z, Uecker R, Irmscher K, et al. Czochralski growth and characterization of β-Ga2O3 single crystals. Cryst Res Technol, 2010, 45(12): 1229. doi: 10.1002/crat.201000341
[61]
Yang J J, Chen H, Liu J X, et al. Ablation characteristics and material removal mechanism of a β-Ga2O3 processed by picosecond laser. Mater Sci Semicond Process, 2024, 173: 108136. doi: 10.1016/j.mssp.2024.108136
[62]
Lenzner M, Krüger J, Kautek W, et al. Incubation of laser ablation in fused silica with 5-fs pulses. Appl Phys A, 1999, 69(4): 465.
[63]
Zhang K, Xu Z W, Dong B, et al. Process exploration of β-Ga2O3 blind hole processing by water-assisted femtosecond laser technology. J Alloys Compd, 2023, 939: 168769. doi: 10.1016/j.jallcom.2023.168769
[64]
Zhang K, Xu Z W, Wang H, et al. Patterning the surface structure of transparent hard-brittle material β-Ga2O3 by ultrashort pulse laser. Ceram Int, 2022, 48(19): 27650. doi: 10.1016/j.ceramint.2022.06.061
[65]
Ahn M, Sarracino A, Ansari A, et al. Unique material modifications of Ga2O3 enabled by ultrafast laser irradiation. Oxide-based Materials and Devices XI, 2020: 20.
[66]
Zhang H B, Eaton S M, Herman P R. Low-loss Type II waveguide writing in fused silica with single picosecond laser pulses. Opt Express, 2006, 14(11): 4826. doi: 10.1364/oe.14.004826
[67]
McMillen B, Zhang B T, Chen K, et al. Ultrafast laser fabrication of low-loss waveguides in chalcogenide glass with 0.65 dB/cm loss. 2012 Conference on Lasers and Electro-Optics (CLEO), 2012: 1.
[68]
Soltani B, Azarhoushang B, Zahedi A. Laser ablation mechanism of silicon nitride with nanosecond and picosecond lasers. Opt Laser Technol, 2019, 119: 105644. doi: 10.1016/j.optlastec.2019.105644
[69]
Wright E M, Koch S W, Kolesik M, et al. Memory effects in the long-wave infrared avalanche ionization of gases: A review of recent progress. Rep Prog Phys, 2019, 82(6): 064401. doi: 10.1088/1361-6633/ab1a07
[70]
Kim T, Bhargava P, Poulton C V, et al. A single-chip optical phased array in a wafer-scale silicon photonics/CMOS 3D-integration platform. IEEE J Solid State Circuits, 2019, 54(11): 3061. doi: 10.1109/JSSC.2019.2934601
[71]
Seok T J, Kwon K, Henriksson J, et al. Wafer-scale silicon photonic switches beyond die size limit. Optica, 2019, 6(4): 490. doi: 10.1364/OPTICA.6.000490
[72]
Lin J J, You T G, Jin T T, et al. Wafer-scale heterogeneous integration InP on trenched Si with a bubble-free interface. APL Mater, 2020, 8(5): 051110. doi: 10.1063/5.0004427
[73]
Hollenbach M, Klingner N, Jagtap N S, et al. Wafer-scale nanofabrication of telecom single-photon emitters in silicon. Nat Commun, 2022, 13: 7683. doi: 10.1038/s41467-022-35051-5
[74]
Jo G, Edinger P, Bleiker S J, et al. Wafer-level hermetically sealed silicon photonic MEMS. Photon Res, 2022, 10(2): A14. doi: 10.1364/PRJ.441215
[75]
Zhang J, Dong P, Dang K, et al. Ultra-wide bandgap semiconductor Ga2O3 power diodes. Nat Commun, 2022, 13: 3900. doi: 10.1038/s41467-022-31664-y
[76]
Labed M, Sengouga N, Prasad C V, et al. On the nature of majority and minority traps in β-Ga2O3: A review. Mater Today Phys, 2023, 36: 101155. doi: 10.1016/j.mtphys.2023.101155
[77]
Sun Z P, Zhang D L, Qi Z J, et al. Insight into interfacial heat transfer of β-Ga(2)O(3)/diamond heterostructures via the machine learning potential. ACS Appl Mater Interfaces, 2024, 16(24): 31666. doi: 10.1021/acsami.3c19588
[78]
Higashiwaki M, Sasaki K, Kuramata A, et al. Development of gallium oxide power devices. Phys Status Solidi A, 2014, 211: 21-26. doi: 10.1002/pssa.201330197
[79]
Shan F K, Liu G X, Lee W J, et al. Structural, electrical, and optical properties of transparent gallium oxide thin films grown by plasma-enhanced atomic layer deposition. J Appl Phys, 2005, 98(2): 023504 doi: 10.1063/1.1980535
[80]
Yoshioka S, Hayashi H, Kuwabara A, et al. Structures and energetics of Ga2O3. J Phys Condens Matter, 2007, 19(34): 346211. doi: 10.1088/0953-8984/19/34/346211
[81]
Roy R, Hill V G, Osborn E F. Polymorphism of Ga2O3 and the system Ga2O3: H2O. J Am Chem Soc, 1952, 74(3): 719.
[82]
Reese S B, Remo T, Green J, et al. How much will gallium oxide power electronics cost? Joule, 2019, 3(4): 903.
[83]
Schaffer C B, Brodeur A, Mazur E. Laser-induced breakdown and damage in bulk transparent materials induced by tightly focused femtosecond laser pulses. Meas Sci Technol, 2001, 12(11): 1784. doi: 10.1088/0957-0233/12/11/305
[84]
Jiang L, Wang A D, Li B, et al. Electrons dynamics control by shaping femtosecond laser pulses in micro/nanofabrication: Modeling, method, measurement and application. Light Sci Appl, 2018, 7(2): 17134. doi: 10.1038/lsa.2017.134
[85]
Chen J L, Lu X Z, Li Z, et al. Anisotropy of material removal during laser-induced plasma assisted ablation of sapphire. Ceram Int, 2022, 48(10): 13880. doi: 10.1016/j.ceramint.2022.01.272
[86]
Lei M L, Meng L H, Lin Y C, et al. Stealth dicing strategy for fabricating the cleavage mirror facets of semiconductor laser. Mater Des, 2025, 251: 113695. doi: 10.1016/j.matdes.2025.113695
[87]
Parks S M, Grote R R, Hopper D A, et al. Fabrication of (111)-faced single-crystal diamond plates by laser nucleated cleaving. Diam Relat Mater, 2018, 84: 20. doi: 10.1016/j.diamond.2018.02.013
[88]
Mu C Y, Lv X Y, Wang Q L, et al. Mosaic growth and characteristics of 2-inch single-crystal diamond. Funct Diam, 2026, 6(1): 2620820. doi: 10.1080/26941112.2026.2620820
[89]
Onishi K, Kitagawa H, Teranishi S, et al. Temporary direct bonding by low temperature deposited SiO2 for chiplet applications. ACS Appl Electron Mater, 2024, 6(4): 2449. doi: 10.1021/acsaelm.4c00114
[90]
Inoue F, Podpod A, Peng L, et al. Morphological characterization and mechanical behavior by dicing and thinning on direct bonded Si wafer. J Manuf Process, 2020, 58: 811. doi: 10.1016/j.jmapro.2020.08.050
[91]
Windemuth R. Plasma dicing for thin wafers. 2015 European Microelectronics Packaging Conference (EMPC), 2016: 1.
[92]
Pushpakaran B N, Subburaj A S, Bayne S B, et al. Impact of silicon carbide semiconductor technology in Photovoltaic Energy System. Renew Sustain Energy Rev, 2016, 55: 971. doi: 10.1016/j.rser.2015.10.161
[93]
Cunningham D W, Carlson E P, Manser J S, et al. Impacts of wide band gap power electronics on photovoltaic system design. IEEE J Photovolt, 2020, 10(1): 213. doi: 10.1109/JPHOTOV.2019.2950592
[94]
Robles E, Matallana A, Aretxabaleta I, et al. The role of power device technology in the electric vehicle powertrain. Int J Energy Res, 2022, 46(15): 22222. doi: 10.1002/er.8581
[95]
Liu G Y, Wu Y B, Li K J, et al. Development of high power SiC devices for rail traction power systems. J Cryst Growth, 2019, 507: 442. doi: 10.1016/j.jcrysgro.2018.10.037
  • Search

    Advanced Search >>

    GET CITATION

    shu

    Export: BibTex EndNote

    Article Metrics

    Article views: 3 Times PDF downloads: 1 Times Cited by: 0 Times

    History

    Received: 30 July 2026 Revised: 08 October 2026 Online: Accepted Manuscript: 24 November 2026

    Catalog

      Email This Article

      User name:
      Email:*请输入正确邮箱
      Code:*验证码错误
      Haoyu Fan, Xing Zhang, Linlin Che, Yufeng Xue, Jiawei Wang, Yangyang Jia, Qiu Chen, Baitao Zhang, Xiufang Chen, Rongkun Wang, Xiangang Xu. Research progress on laser stealth dicing of typical semiconductor materials[J]. Journal of Semiconductors, 2026, In Press. doi: 10.1088/1674-4926/26070048 ****H Y Fan, X Zhang, L L Che, Y F Xue, J W Wang, Y Y Jia, Q Chen, B T Zhang, X F Chen, R K Wang, and X G Xu, Research progress on laser stealth dicing of typical semiconductor materials[J]. J. Semicond., 2026, accepted doi: 10.1088/1674-4926/26070048
      Citation:
      Haoyu Fan, Xing Zhang, Linlin Che, Yufeng Xue, Jiawei Wang, Yangyang Jia, Qiu Chen, Baitao Zhang, Xiufang Chen, Rongkun Wang, Xiangang Xu. Research progress on laser stealth dicing of typical semiconductor materials[J]. Journal of Semiconductors, 2026, In Press. doi: 10.1088/1674-4926/26070048 ****
      H Y Fan, X Zhang, L L Che, Y F Xue, J W Wang, Y Y Jia, Q Chen, B T Zhang, X F Chen, R K Wang, and X G Xu, Research progress on laser stealth dicing of typical semiconductor materials[J]. J. Semicond., 2026, accepted doi: 10.1088/1674-4926/26070048

      Research progress on laser stealth dicing of typical semiconductor materials

      DOI: 10.1088/1674-4926/26070048
      CSTR: 32376.14.1674-4926.26070048
      More Information
      • Haoyu Fan received his B.Eng. degree from Shandong University of Science and Technology, China, in 2024. He is currently pursuing his Ph.D. degree through an integrated master's–doctoral program at Shandong University, China. His research interests mainly focus on semiconductor laser processing
      • Rongkun Wang is an Associate Research Professor and Ph.D. supervisor at Shandong University, China. He is a Taishan Young Scholar and a Xiaomi Young Scholar. His research interests focus on laser ultraprecision processing of semiconductor materials, particularly silicon carbide (SiC), and the development of high-power semiconductor laser chips and pump sources
      • Corresponding author: chenqiu0629@sdu.edu.cn; cxf@sdu.edu.cn; wrk@sdu.edu.cn
      • Received Date: 2026-07-30
      • Revised Date: 2026-10-08
      • Available Online: 2026-11-24

      Catalog

        /

        DownLoad:  Full-Size Img  PowerPoint
        Return
        Return